410 vs 410S vs 420 Stainless Steel

Order 410 stainless steel when the part needs strength after hardening, 410S when the part is welded or formed and needs no hardening, and 420 stainless steel when it needs a hard edge or a wear surface. All three are straight-chromium steels with 11.50 to 14.00 percent chromium. Nickel is limited to 0.75 percent maximum in 410 and 420, and to 0.60 percent maximum in 410S.

410, 410S and 420 at a glance

Carbon, %, scale 0 to 0.40 %

4100.08 to 0.15
410S0.08 max
4200.15 to 0.40

Typical hardened hardness, HRC, scale 0 to 60 HRC

41038 to 45
410Shardens very little
42053 to 57

Choose 410 for

  • Valves, shafts, fasteners, pump components
  • Cutlery blanks

Choose 410S for

  • Welded or formed general-purpose parts
  • Tower packing, distillation trays, exhaust components

Choose 420 for

  • Knives, cutting tools, surgical instruments
  • Wear-resistant parts
Carbon for 420 is the datasheet range. Hardened hardness is typical producer data, not a limit: 410 at 0.14 % carbon, 420 at 0.38 % carbon.

Carbon decides the 410 vs 410S vs 420 stainless steel choice. 410 holds 0.08 to 0.15 percent carbon, 410S holds 0.08 percent maximum, and 420 holds 0.15 percent minimum. Typical hardened 410 measures 38 to 45 HRC, and typical hardened 420 measures 53 to 57 HRC. 410S hardens very little.

410 and 420 are martensitic, and 410S is ferritic when annealed. All three are magnetic. Corrosion resistance of 410 and 420 is moderate and depends on the condition of the part and on cleaning. Welding favours 410S, because its low carbon helps prevent cracking. Minimum tensile strength runs from 415 MPa for 410S to 450 MPa for 410 and 690 MPa for 420.

What Are 410, 410S and 420 Stainless Steel?

SS 410 and SS 420 are martensitic stainless steels that harden by heat treatment, and 410S is a low-carbon modification of 410 that is ferritic when annealed.

Straight-chromium means chromium is the main alloying element and nickel is nearly absent. Martensitic describes a steel that hardens when it is heated and quenched, which means cooled fast. Ferritic describes the structure of 410S after annealing, which means softening by heat. Low carbon limits how far 410S stainless steel (UNS S41008) can harden. 410 carries UNS S41000, and 420 carries UNS S42000.

Designation410410S420
TypeMartensiticFerritic when annealedMartensitic
UNSS41000S41008S42000
EN number1.40061.40001.4021
JISSUS410SUS410Snot listed
ISX12Cr12X04Cr12X20Cr13

UNS is the Unified Numbering System, EN is the European standard, JIS is the Japanese Industrial Standard and IS is the Indian Standard.

Chemical Composition of 410, 410S and 420

The grades differ mainly in carbon and nickel: 410 has 0.08 to 0.15 percent carbon, 410S has 0.08 percent maximum, and 420 has 0.15 percent minimum.

Element410410S420
C (Carbon)0.08 to 0.150.08 max0.15 min
Cr (Chromium)11.50 to 13.5011.50 to 13.5012.00 to 14.00
Ni (Nickel)0.75 max0.60 max0.75 max
Mn (Manganese)1.00 max1.00 max1.00 max
Si (Silicon)1.00 max1.00 max1.00 max
P (Phosphorus)0.040 max0.040 max0.040 max
S (Sulphur)0.030 max0.030 max0.030 max

All values in % by weight.

420 has no carbon maximum in the specification values, and the producer datasheet gives 0.15 to 0.40 percent. 420 holds 0.50 percent more chromium than 410 at both limits and also limits molybdenum to 0.50 percent maximum.

ASTM A240/A240M covers plate, sheet and strip of chromium stainless steels, and a producer lists it for 410 and 410S. No standard is named for 420 here, and its values are producer specification values.

How Do 410, 410S and 420 Harden?

410 and 420 harden by heating and quenching, and 420 hardens further because it holds more carbon, while 410S hardens very little because its carbon is low.

The hardening temperature is 982 °C for 410 and 1010 to 1066 °C for 420. The part is quenched in oil, or air cooled when the section is thin. Quenched martensite is quite brittle, so the part is then tempered. Tempering means reheating a hardened part at a lower temperature to restore some ductility. Hardness and strength change very little with tempering temperatures up to 482 °C.

GradeCarbon in the tested steel (%)Typical hardened hardness
4100.1438 to 45 HRC
4200.3853 to 57 HRC

HRC is the Rockwell C hardness scale used for hard steel. The values are typical producer data, not limits.

410S stays soft and ductile even when it is cooled rapidly from above the critical temperature. That low hardening helps prevent cracking when the steel is welded. 410S is completely ferritic in the annealed condition.

Mechanical Properties and Hardness Compared

420 has the highest minimum tensile strength at 690 MPa, against 450 MPa for 410 and 415 MPa for 410S.

Property410410S420
Tensile strength450 MPa min415 MPa min690 MPa min
Yield strength205 MPa min205 MPa minnot listed
Elongation20 % min22 % min15 % min
Hardness limit96 HRB max89 HRB max96 HRB max
Typical annealed hardness82 HRBnot listed87 HRB

HRB is the Rockwell B scale used for softer steel. The tensile, yield, elongation and hardness limits are specification values. The annealed hardness values are typical, not limits. Annealed 410 also measures 126 to 192 on the Brinell scale (HB).

Hardness follows carbon, so 420 reaches greater hardness than 410. 410 gives moderate hardness with good strength.

Are 410, 410S and 420 Magnetic?

Yes, 410, 410S and 420 are all magnetic.

Martensitic grades such as 410 and 420 show pronounced magnetism. The producer datasheet for 410S lists it as ferromagnetic, which means it is strongly attracted by a magnet.

A magnet alone does not identify the grade. All three attract a magnet, so a magnet cannot separate one from another. The chemical analysis on the mill test certificate shows carbon and chromium for the heat, and that identifies the grade.

Corrosion Resistance of 410, 410S and 420

410 and 420 resist atmospheric corrosion, potable water and mildly corrosive chemicals, but they resist less than austenitic or duplex grades.

Contact with chlorides in everyday use is generally satisfactory when the part is cleaned properly after exposure. Chlorides occur in seawater and in process solutions.

Producer data do not agree on which of 410 and 420 resists corrosion better, so we give no ranking. Resistance depends on the condition of the part and on cleaning. No ranking is given for 410S either.

The pitting resistance number (PREN) adds chromium, molybdenum and nitrogen as %Cr + 3.3 x %Mo + 16 x %N. Molybdenum and nitrogen are counted as zero, because no minimum is specified.

GradeChromium minimum (%)PREN (calculated from minimum composition)
41011.5011.5
410S11.5011.5
42012.0012.0

PREN is a rough comparison only, and it gives no information on behaviour in real environments. The same method gives 17.5 for 304 and 22.6 for 316, so chloride service is a grade-review case. The stainless steel grade selector narrows the choice.

Welding and Machining 410, 410S and 420

410S suits welded and formed parts, because its low carbon helps prevent cracking when the steel is welded.

410 and 410S are easier to form, weld and machine than higher-carbon martensitic grades such as 420. Martensitic grades have limited weldability and often need preheating or post-weld treatment.

410 and 420 are machined in the annealed condition.

Uses of 410, 410S and 420

410 is used for valves, fasteners, shafts, pump components, cutlery blanks and industrial tools; 410S for general-purpose components; and 420 for knives, surgical instruments, cutting tools and wear-resistant parts.

GradeUses
410valves, fasteners, shafts, pump components, cutlery blanks, industrial tools, structural and industrial components
410Sgeneral-purpose components where fabrication ease is important; tower packing, distillation trays, automotive exhaust components, other high-temperature applications
420knives, surgical instruments, cutting tools, wear-resistant parts

Cutlery is a major use of the 410 and 420 family. The family is also used for dental instruments, nozzles, hardened steel balls and seats for oil well pumps, separating screens and strainers, springs, shears and wear surfaces.

Limits for hot service depend on the atmosphere and the load, so no single temperature is printed for any of the three grades.

How to Choose Between 410, 410S and 420

Choose 410 for strength with hardening, 410S for welded or formed parts that need no hardening, and 420 for edges and wear surfaces.

JobGrade to order
Valves, shafts, fasteners, pump components410
Cutlery blanks410
Welded or formed general-purpose parts410S
Tower packing, distillation trays, exhaust components410S
Knives, cutting tools, surgical instruments420
Wear-resistant parts420
Chloride or acid serviceGrade review, send the duty
Hot serviceGrade review, send the duty

Each grade page shows the current indicative price: 410 stainless steel sheets and plates, 410S stainless steel sheets and plates and 420 stainless steel sheets and plates. Coil is on the 410 stainless steel coils, 410S coils and 420 coils pages.

A mill test certificate comes with every supply. The certificate reports the heat chemical analysis and the mechanical test results, so the carbon and chromium can be compared with the limits above. Magnetic chromium grades outside this family, such as 430, are set against 304 in 430 compared with 304.

An enquiry needs the grade, thickness, width, length, quantity and end use. Buyers can send the service conditions to us, including temperature and atmosphere for a hot or wet duty, and we will check the grade against them.

Frequently Asked Questions

What Is the Main Difference Between 410 and 410S?

The main difference is carbon: 410 holds 0.08 to 0.15 percent and hardens by quenching, while 410S holds 0.08 percent maximum and hardens very little. 410S is a low-carbon modification of 410 and stays ferritic when annealed. Its nickel limit is also lower, at 0.60 percent against 0.75 percent.

How Much Does 410S Harden?

410S hardens very little, because its low carbon restricts the ability to harden. The material remains soft and ductile even when it is cooled rapidly from above the critical temperature. That helps prevent cracking when the steel is welded.

Is 420 Harder Than 410?

Yes, 420 reaches higher hardness because it holds more carbon. Typical hardened 420 with 0.38 percent carbon measures 53 to 57 HRC, against 38 to 45 HRC for typical hardened 410 with 0.14 percent carbon. Annealed, typical 420 measures 87 HRB and typical 410 measures 82 HRB.

Which Is Used for Cutlery, 410 or 420?

Both are used, because cutlery is a major use of the 410 and 420 family. 410 serves cutlery blanks, and 420 serves knives and cutting tools, where higher hardness is needed.

What Is the Maximum Service Temperature of 410, 410S and 420?

No single figure applies to the three grades, because the limit depends on the atmosphere and the load. Jindal states 650 °C continuous for its 410, and we found no official figure for 410S or 420. Send us the duty and we will check it. Heat-resisting grades with stated scaling and service figures are compared in 309S vs 310S stainless steel.

Which Standard Covers 410, 410S and 420?

ASTM A240/A240M covers plate, sheet and strip of chromium stainless steels, and a producer lists it for 410 and 410S. No standard is named for 420, and its values are producer specification values. State the standard and the condition on the enquiry.

Can 410S Replace 410 in a Hardened Part?

No, 410S hardens very little, so it does not replace 410 where the part must be hardened. Where the part is welded or formed and stays annealed, 410S is the low-carbon form to specify.