A stainless steel grade selector matches a grade to its service condition in a fixed order: environment, temperature, strength, welding and cost. Corrosion decides most choices. SS 304 covers interior and light urban air, 316 covers coastal and polluted air, and 904L, 2205 and S32750 cover acids and high chlorides. 310S covers furnace heat, and 430, 201 and 202 cover low-cost indoor work. Strength then narrows the list, since 2205 has 450 MPa minimum yield strength. Welded parts call for the low carbon grades 304L and 316L. Cost follows nickel and molybdenum content, so the low-nickel grades cost least.
From service condition to grade
- Environment
- Temperature
- Strength
- Welding
- Budget
Interior, decorative, low cost
430201202
General use, food, kitchen
304
Welded fabrication
304L316L
Coastal and chloride air
316316L
Strength with chlorides
2205
Acids
904L
High chlorides, offshore
S32750
Furnace heat
310S
How Do I Choose a Stainless Steel Grade?
Stainless steel grade selection follows five questions, asked in this order:
- Name the environment: indoor air, urban air, coastal air, fresh water, a chloride solution or an acid.
- Name the temperature, both the working range and any welding heat.
- Name the strength needed, as minimum yield strength in MPa.
- State whether the part is welded and whether it is annealed afterwards.
- Set the budget last, because nickel and molybdenum content drive the price.
A grade is the alloy designation, such as 304, 316L or 2205. Annealed austenitic stainless steel, which includes 304 and 316, shows no magnet pull. Ferritic 430 is magnetic. Duplex grades such as 2205 have about twice the yield strength of 304.
Stepping up a grade costs money and gains nothing in a mild environment. 304 is enough for interior and light urban air, so 316 is not needed there.
Stainless Steel Grade Selector Table
The grade selector table matches eight requirements to the grades that fit and the reason each fits.
| Requirement | Grades | Why |
|---|---|---|
| Interior, decorative, low cost | 430, 201, 202 | Little or no nickel keeps the price down; indoor, low-corrosion use |
| General use, food, kitchen | 304 | Covers interior and light urban air; the most specified grade |
| Welded fabrication | 304L, 316L | Carbon 0.030 % max; post-weld annealing generally not needed |
| Coastal and chloride air | 316, 316L | 2.00 to 3.00 % molybdenum resists chlorides better than 304 |
| Strength with chlorides | 2205 | Yield 450 MPa min; PREN about 35 |
| Acids | 904L | 4.00 to 5.00 % molybdenum and 1.00 to 2.00 % copper |
| High chlorides, offshore | S32750 | PREN above 40; yield 550 MPa min |
| Furnace heat | 310S | 1050 °C maximum service temperature in air, intermittent |
Grade Selection Examples by Service
The five questions give one grade for each service, with the reason taken from the grade limits.
| Service | Deciding question | Grade | Reason |
|---|---|---|---|
| Kitchen equipment in an interior | Environment | 304 | Covers interior and light urban air |
| Welded tank in a chemical or food plant | Welding | 304L | Carbon 0.030 % max; post-weld annealing generally not needed |
| Boat fittings and deck hardware | Environment | 316 | 2.00 to 3.00 % molybdenum resists chlorides |
| Offshore seawater piping | Environment and strength | S32750 | PREN above 40; yield 550 MPa min; avoid prolonged exposure above 250 °C |
| Sulphuric acid service in a chemical plant | Environment | 904L | 4.00 to 5.00 % molybdenum and 1.00 to 2.00 % copper |
| Furnace parts and kilns | Temperature | 310S | 1050 °C maximum service temperature in air, intermittent |
Which Grade Suits General Use?
SS 304 suits general use: interior and light urban air, kitchen equipment, food-handling equipment, sinks and appliances. Grade 304 is the most specified stainless steel, with more than half of world stainless production. Grade 304 contains 17.5 to 19.5 percent chromium and 8.0 to 10.5 percent nickel.
Other uses of 304 stainless steel include dairy equipment, handrails, revolving doors and architectural fittings. Annealed 304 shows no magnet pull, while welded 304 often attracts a magnet lightly. A magnet alone therefore does not identify the grade.
Buyers who compare it with cheaper grades can read the 201 vs 202 vs 304 comparison and the 430 vs 304 comparison. Full specifications sit on the 304 stainless steel sheets and plates page.
Which Grade Resists Chlorides and Coastal Air?
316 and 316L resist chlorides better than 304 because they contain 2.00 to 3.00 percent molybdenum. Chlorides are salts, found in seawater and process solutions, and they cause pitting and crevice corrosion in stainless steel. Chlorides are also the primary driver of atmospheric corrosion, and coastal and urban areas are particularly aggressive.
316 and 316L are used for urban air, including light marine-influenced or polluted settings. Uses include boat fittings, deck hardware and coastal architectural components. 316L sheets and plates are the welded version of the grade. 304 and 316 can suffer stress corrosion cracking in chloride environments above about 50 °C under tensile stress. The 304 vs 316 comparison sets the two grades side by side.
PREN Comparison of Stainless Steel Grades
PREN, the pitting resistance equivalent number, ranks pitting resistance as PREN = %Cr + 3.3 x %Mo + 16 x %N, where Cr is chromium, Mo is molybdenum and N is nitrogen. A higher PREN means higher resistance to pitting in chlorides.
| Grade | PREN calculated from minimum composition | Producer figure |
|---|---|---|
| 201 | 16.0 | Not stated |
| 202 | 17.0 | Not stated |
| 430 | 16.0 | Not stated |
| 304 and 304L | 17.5 | Not stated |
| 316 and 316L | 22.6 | Not stated |
| 904L | 32.2 | 34 minimum |
| 2205 | 34.1 | about 35 |
| S32750 | 37.7 | above 40 |
PREN gives only an indication of resistance and says nothing about behaviour in a real environment, so the figures are a rough comparison. The PREN calculator calculates the number from your own composition.
Duplex and Super Duplex for High Chlorides
Duplex 2205 and super duplex S32750 are chosen when chlorides and strength both matter. 2205 is used in desalination, pulp and paper, and chemical tanks. Super duplex and super austenitic grades can handle high-chloride environments up to nearly boiling point. S32750 is used for offshore heat exchangers, seawater piping and high-pressure reverse osmosis desalination.
Both grades are covered on the duplex 2205 sheets and plates and super duplex S32750 plates pages. A fuller comparison sits in the guide to stainless grades for seawater and chloride service.
Which Grade Handles Acids?
904L handles acid service, including sulphuric acid, phosphoric acid and mixed acid solutions in chemical plants. The grade contains 23.00 to 28.00 percent nickel, 4.00 to 5.00 percent molybdenum and 1.00 to 2.00 percent copper, with carbon at 0.02 percent maximum.
The 904L page lists acid limits: sulphuric acid at 0 to 100 percent up to about 35 °C, and hydrochloric acid only at 1 to 2 percent. Other uses are fertiliser plants, flue gas desulphurisation, pulp bleaching and pharmaceutical processing. Details are on the 904L sheets and plates page and in the guide to stainless steel for chemical plants.
904L is not needed for general atmospheric conditions. 304 or 316L gives adequate service there at a lower price.
Which Grade Withstands Heat?
310S is the furnace-heat grade, with a maximum service temperature in air of 1050 °C for intermittent heating. The table gives each temperature figure with what it means.
| Grade | Figure | What it means |
|---|---|---|
| 310S | 1050 °C | Maximum service temperature in air |
| 310S | 1093 °C | Resists scaling up to this temperature |
| 309S | 1090 °C | Oxidation resistance up to this temperature |
| 904L | -60 to +400 °C | Service temperature range |
| 2205 | -40 to 300 °C | Service temperature range |
| S32750 | 250 °C | Avoid prolonged exposure above this |
Scaling means oxidation of the metal surface at heat. 310S sheets and plates suit furnace parts, kilns, radiant tubes and annealing covers. 309S sheets and plates suit furnace components, boiler baffles and refinery equipment under thermal cycling.
No single temperature applies to 304 or 316. The limit depends on the grade, the design code and the atmosphere, so send us the duty and we confirm the grade.
Which Grade Gives Higher Strength?
2205 has 450 MPa minimum yield strength, about twice the 205 MPa of 304. S32750 reaches 550 MPa. The table compares the grades on the two strength limits.
| Grade | Tensile strength (MPa min) | Yield strength (MPa min) |
|---|---|---|
| 430 | 450 | 205 |
| 304L, 316L | 485 | 170 |
| 904L | 490 | 220 |
| 304, 316 | 515 | 205 |
| 202 (mill specification) | 620 | 260 |
| 201 (type 201-2) | 655 | 310 |
| 2205 | 655 | 450 |
| S32750 | 795 | 550 |
Which Grade Suits Welded Fabrication?
304L and 316L suit welded fabrication because both limit carbon to 0.030 percent maximum. Low carbon minimises chromium carbide formation during welding. Tanks, pressure vessels and welded structures in chemical and food industries use 304L.
316 holds 0.08 percent carbon maximum and needs post-weld annealing to restore corrosion resistance, mainly in heavy sections. 321 is titanium-stabilised and is chosen for superior resistance to intergranular corrosion. Austenitic grades are highly weldable. 430 can be welded, but welding it is more challenging.
The guide to 304L and 316L low carbon grades explains carbon limits and certificates. The 321 sheets page covers the stabilised grade.
Which Grade Costs Less?
430, 201 and 202 cost less than 304 because they hold little nickel, and 316 costs more than 304 because of its molybdenum. 430 holds 0.75 percent nickel at most. 202 uses 4.0 to 6.0 percent nickel against 8.0 to 10.5 percent in 304. 316 contains 2.00 to 3.00 percent molybdenum, which 304 does not specify.
904L costs more than 316 in the indicative market range, since it holds 23.00 to 28.00 percent nickel and 4.00 to 5.00 percent molybdenum.
A low price brings lower corrosion resistance. 200-series grades have less corrosion resistance than 304, and failures have occurred in some applications. 202 suits budget, indoor, low-corrosion projects. 201 sheets and plates, 202 sheets and plates and 430 sheets and plates carry the details. The 316 sheets and plates page and the stainless steel sheet price per kg page give the current indicative range.
Frequently Asked Questions
Which Stainless Steel Grade Is Magnetic?
430 is magnetic. Annealed austenitic grades such as 304 show no magnet pull, but welded 304 often attracts a magnet lightly, and cold work can add weak attraction. A magnet test alone does not identify a grade.
Is 316 Worth the Extra Cost Over 304?
Yes, in coastal, polluted or chloride service, where its 2.00 to 3.00 percent molybdenum resists pitting. No, in interior and light urban air, where 304 gives adequate service. The extra cost comes from that molybdenum.
Is 201 Suitable for Outdoor Use?
No, 201 suits indoor, low-corrosion use such as small appliances, catering equipment and cooking utensils. Its corrosion resistance is comparable to 301-grade and below 304. Outdoor air in coastal and urban areas carries chlorides, so 304 is the choice in light urban air and 316L in coastal and polluted air.
Does a Higher PREN Always Mean a Better Grade?
No, PREN gives only an indication of pitting resistance and says nothing about behaviour in a real environment. Use it as a rough comparison between grades, then check the service. Chlorides, temperature and surface deposits matter most for pitting and crevice corrosion.
When Do I Need Duplex Stainless Steel?
Duplex stainless steel is needed when a part meets chlorides and needs high strength together. 2205 gives 450 MPa minimum yield and a PREN of about 35. S32750 gives PREN above 40, and prolonged exposure above 250 °C should be avoided.
What Is the Maximum Temperature for Stainless Steel?
The maximum temperature depends on the grade, the design code and the atmosphere, so no single figure applies. 310S has 1050 °C maximum service temperature in air, intermittent. 2205 is rated -40 to 300 °C. Send the duty and we confirm the grade.
Ask Us to Confirm Your Grade
We confirm the grade against your service before we quote. Send the medium and its concentration, the working temperature, whether the part is welded, the thickness and size, and the quantity to info@ostravametals.com or through the contact page. We cut sheets and plates to size and issue a mill test certificate with every supply. The full range is on the stainless steel sheets and plates page.