Skip to content
Ostrava Metals

Welding and L grades

L Grades Explained: 304 vs 304L and 316 vs 316L

In the 304 vs 304L choice, and in 316 vs 316L, the L stands for low carbon: both L grades limit carbon to 0.030 percent maximum, against 0.07 percent for 304 and 0.08 percent for 316. Carbon matters in welding, because chromium carbides can form at grain boundaries and reduce corrosion resistance. That damage is called sensitisation, and its problem zone runs from 450 to 850 °C. The L grades carry lower strength minimums: 485 MPa tensile against 515 MPa. Dual certified material is intended to meet both grades on one certificate.

Carbon limit, standard and L grades

Carbon, % max, scale 0 to 0.10 %

3040.07 max
304L0.030 max
3160.08 max
316L0.030 max

Choose 304L or 316L for

  • Tanks, pressure vessels and welded structures in chemical and food industries
  • Extensive welding in pharmaceutical manufacturing and food processing
  • Welded structures in marine environments
  • Biomedical implants, including orthopaedic implants

Choose 304 or 316 for

  • Unwelded parts such as utensils, cookware, sinks and appliances
  • Surgical instruments, medical devices, boat fittings and deck hardware
Low carbon limits carbide formation in the 450 to 850 °C zone during welding. The L grades carry 485 MPa minimum tensile strength against 515 MPa.

What Does the L Mean in 304L and 316L?

The L in 304L and 316L stands for low carbon: both grades limit carbon to 0.030 percent maximum. Standard 304 allows 0.07 percent maximum carbon and 316 allows 0.08 percent maximum. Low carbon 304 is another name for 304L.

Chromium, nickel and molybdenum limits stay close in each pair. Each grade also carries a Unified Numbering System (UNS) number, the standard alloy code used on certificates.

GradeUNSCarbon (% max)Chromium (%)Nickel (%)Molybdenum (%)
304S304000.0717.5 to 19.58.0 to 10.5Not specified
304LS304030.03017.5 to 19.58.0 to 12.0Not specified
316S316000.0816.00 to 18.0010.00 to 14.002.00 to 3.00
316LS316030.03016.00 to 18.0010.00 to 14.002.00 to 3.00

What Is Sensitisation in Stainless Steel?

Sensitisation is the formation of chromium carbides at grain boundaries, which reduces corrosion resistance. Grain boundaries are the edges between the crystals of the metal. Attack along them is called intergranular corrosion.

The problem temperature zone is 450 to 850 °C, where sensitisation risk arises during welding or service. SS 304L has low carbon, which minimises carbide formation during welding. In 316, higher carbon can cause precipitation at high temperatures, and that can reduce corrosion resistance in welded areas.

316 therefore needs post-weld annealing to restore corrosion resistance, mainly in heavy sections. Post-weld annealing means heating the finished weld to restore the metal. 316L allows excellent weldability without post-weld heat treatment. Low carbon reduces the risk of sensitisation, but no L grade should be described as immune.

When Should I Choose 304L or 316L?

Choose 304L when welding is unavoidable or the environment is corrosive, and choose 316L for extensive welding or corrosive service where post-weld heat treatment is not possible. The table maps the uses to the grade.

ConditionGradeWhy
Tanks, pressure vessels and welded structures in chemical and food industries304LCarbon 0.030 % max; post-weld annealing generally not needed
Extensive welding in pharmaceutical manufacturing and food processing316LCarbon 0.030 % max; no post-weld heat treatment
Welded structures in marine environments316L2.00 to 3.00 % molybdenum for chloride resistance
Biomedical implants, including orthopaedic implants316LLow carbon with molybdenum
Utensils, cookware, sinks and appliances304Unwelded parts; carbon 0.07 % max is acceptable
Surgical instruments, medical devices, boat fittings and deck hardware3162.00 to 3.00 % molybdenum for chlorides

Does Thickness Decide the Grade?

No, thickness alone does not decide the grade. L grades are often available in thicker sizes, greater than about 5 mm in flat products. That is a stock note, not a rule that thin sheet needs no L grade.

Standard 304 serves unwelded parts such as utensils, cookware and sinks, and 316 serves surgical instruments and boat fittings. The 304 sheets and plates and 316 sheets and plates pages carry their specifications.

Is 304L Weaker Than 304?

Yes, slightly: 304L has 485 MPa minimum tensile strength and 170 MPa minimum yield strength, against 515 MPa and 205 MPa for 304. The same gap applies to 316L against 316.

GradeTensile strength (MPa min)Yield strength (MPa min)Elongation (% min)Hardness (HRB max)
3045152054092
304L4851704092
3165152054095
316L4851704095

The gap is 30 MPa in tensile strength and 35 MPa in yield strength. Higher carbon in 316 gives somewhat higher tensile and yield strength than 316L. Mills generally ensure that L-grade heats meet the strength requirements of the standard grade, which is why dual certified material exists.

Does 304L Resist Corrosion Better Than 304?

No, the L grade does not raise pitting resistance: 304 and 304L share the same chromium limits and the same calculated PREN of 17.5. PREN, the pitting resistance equivalent number, is calculated as %Cr + 3.3 x %Mo + 16 x %N, where Cr is chromium, Mo is molybdenum and N is nitrogen.

GradePREN calculated from minimum composition
30417.5
304L17.5
31622.6
316L22.6

Carbon does not enter the formula. The L grade protects the weld and the metal beside it, while molybdenum raises chloride resistance: 316 and 316L contain 2.00 to 3.00 percent. PREN gives only an indication of resistance and says nothing about behaviour in a real environment. The PREN calculator works out the number for other compositions, and the 304 vs 316 comparison covers the molybdenum gap.

How Do 316 and 316L Differ in Use?

316 and 316L differ only in carbon, since every other composition limit is the same. Both contain 16.00 to 18.00 percent chromium, 10.00 to 14.00 percent nickel and 2.00 to 3.00 percent molybdenum.

Property316316L
Carbon (% max)0.080.030
Tensile strength (MPa min)515485
Yield strength (MPa min)205170
After weldingPost-weld annealing, mainly heavy sectionsNo post-weld heat treatment
UsesChemical processing equipment, petrochemical, oil and gas, surgical instruments, medical devices, boat fittings, deck hardwarePharmaceutical manufacturing, food processing, biomedical implants, welded marine structures

What Is Dual Certified 304/304L Stainless Steel?

Dual certified 304/304L is one product intended to meet the requirements of both 304 and 304L. Dual certified 316/316L works the same way for 316 and 316L.

A dual certified product must show the stricter value of each pair. Check a dual certificate in four steps:

  1. Confirm the certificate names both grades.
  2. Check carbon at 0.030 percent maximum or lower.
  3. Check tensile strength at 515 MPa minimum or higher.
  4. Check yield strength at 205 MPa minimum or higher.

A dual certified product cannot replace an H grade, which must be specified at order. Our mill test certificate page describes the documents that come with each supply.

How Do 304L and 316L Prices Compare With 304 and 316?

The sheet rates of 304L overlap those of 304, and the rates of 316L overlap those of 316, in the indicative market range. Form, thickness, finish and quantity also move the rate. Molybdenum sets the larger gap, since 316 and 316L contain 2.00 to 3.00 percent molybdenum and 304 and 304L specify none.

316 costs more than 304 because of that molybdenum. Current rates for the L grades are on the 304L sheets and plates and 316L sheets and plates pages, and the indicative range is on the stainless steel sheet price per kg page.

Frequently Asked Questions

Can I Use 304 for Welded Parts?

Yes, 304 can be welded, since austenitic grades are highly weldable. 304L is the grade chosen when welding is unavoidable or the service is corrosive. The stainless steel grade selector places both grades among the other service conditions.

Is 304L Magnetic?

No, annealed austenitic stainless steel such as 304L shows no magnet pull. Welded 304 often attracts a magnet lightly even though the base metal is non-magnetic. A magnet alone does not identify the grade.

Can 316L Replace 316?

Yes, when the specification accepts the lower strength minimums of 316L: 485 MPa tensile and 170 MPa yield, against 515 MPa and 205 MPa for 316. Dual certified 316/316L covers both specifications on one certificate.

Does 304L Need Post-Weld Annealing?

No, 304L generally does not need post-weld annealing, because its carbon is limited to 0.030 percent maximum. Standard 316 with 0.08 percent maximum carbon needs it, mainly in heavy sections.

Is 316L Suitable for Marine Use?

Yes, SS 316L is used for welded structures in marine environments because its 2.00 to 3.00 percent molybdenum resists chlorides. Severe seawater service needs a higher PREN, covered in the guide to stainless grades for seawater and chloride service.

Are the L Grades Immune to Sensitisation?

No, low carbon reduces the risk of sensitisation, but no L grade should be described as immune. The problem temperature zone of 450 to 850 °C still applies during welding or service.

Does 304L Meet the Strength of 304?

No, 304L is specified lower: 485 MPa tensile and 170 MPa yield, against 515 MPa and 205 MPa for 304. Mills generally ensure that L-grade heats meet the strength requirements of the standard grade, which is why dual certified material exists.

What Should I Write in an Enquiry for L Grades?

State the grade as 304L, 316L or dual certified 304/304L, then the form, thickness, finish, quantity and whether the part is welded. Ask for a mill test certificate that shows carbon, tensile and yield values.

Order 304L and 316L Sheets and Plates

We cut 304L and 316L sheets and plates to size and issue a mill test certificate with every supply. Send the grade, thickness, size, quantity and welding duty to info@ostravametals.com or through the contact page, and we reply with the offer.

Contact Ostrava Metals