310S stainless steel suits furnaces, kilns and radiant tubes that need the higher chromium and nickel, and 309S suits furnace equipment, annealing boxes and baffle plates. 310S holds 24.00 to 26.00 percent chromium and 19.00 to 22.00 percent nickel. 309S holds 22.00 to 24.00 percent chromium and 12.00 to 15.00 percent nickel.
309S, 310S and 310 at a glance
Chromium, % by weight, scale 0 to 30 %
Nickel, % by weight, scale 0 to 30 %
- 309S, oxidation resistance up to
- 1090 °C, not a service limit
- 309S, maximum application temperature in air
- 1000 °C, producer guidance
- 310S, resists scaling up to
- 1093 °C, not a maximum temperature
- 310S, maximum service temperature in air
- 1050 °C, suits intermittent heating
Choose 309S for
- Furnace equipment, annealing boxes, baffle plates, thermowells
Choose 310S for
- Furnaces, kilns, radiant tubes, burner parts
- Intermittent high-temperature use
The S means low carbon, 0.08 percent maximum, and it improves weldability. 310 differs from 310S only in carbon, which it allows up to 0.25 percent maximum. All three grades share a minimum tensile strength of 515 MPa.
Temperature figures measure different things. 310S resists scaling up to 1093 °C and has a maximum service temperature in air of 1050 °C. 309S shows oxidation resistance up to 1090 °C, and a producer gives 1000 °C as its maximum application temperature in air. In the 309S vs 310S stainless steel choice, the atmosphere and the load set the real limit.
What Are 309S, 310S and 310 Stainless Steel?
309S, 310S and 310 are austenitic heat-resisting stainless steels, which are chromium-nickel grades for service above about 550 °C.
Austenitic describes chromium-nickel stainless steels. Above about 550 °C creep strength usually sets the design. Creep is the slow stretching of metal under load at high temperature. A producer describes 309S stainless steel (UNS S30908) as an austenitic grade with improved oxidation resistance, and 310S carries UNS S31008.
| Designation | 309S | 310S | 310 |
|---|---|---|---|
| UNS | S30908 | S31008 | S31000 |
| EN number | 1.4833 | 1.4845 | not listed |
| JIS | SUS309S | SUS310S | not listed |
UNS is the Unified Numbering System, EN is the European standard and JIS is the Japanese Industrial Standard. Plain 309 carries UNS S30900.
What Does the S Mean in 309S and 310S?
The S in 309S and 310S means low carbon: both grades limit carbon to 0.08 percent maximum.
Plain 309 allows 0.20 percent carbon maximum, and plain 310 allows 0.25 percent maximum. A producer states that the reduced carbon of 309S improves weldability. For SS 310S, the producer states that the low carbon improves weldability and resistance to intergranular corrosion, which is corrosion along the boundaries between the metal's grains.
Chemical Composition of 309S, 310S and 310
310S holds 24.00 to 26.00 percent chromium and 19.00 to 22.00 percent nickel, against 22.00 to 24.00 percent chromium and 12.00 to 15.00 percent nickel in 309S.
| Element | 309S | 310S | 310 |
|---|---|---|---|
| C (Carbon) | 0.08 max | 0.08 max | 0.25 max |
| Mn (Manganese) | 2.00 max | 2.00 max | 2.00 max |
| Si (Silicon) | 0.75 max | 1.50 max | 1.50 max |
| P (Phosphorus) | 0.045 max | 0.045 max | 0.045 max |
| S (Sulphur) | 0.030 max | 0.030 max | 0.030 max |
| Cr (Chromium) | 22.00 to 24.00 | 24.00 to 26.00 | 24.0 to 26.0 |
| Ni (Nickel) | 12.00 to 15.00 | 19.00 to 22.00 | 19.0 to 22.0 |
All values in % by weight.
The chromium ranges meet at 24.00 percent. The nickel minimum of 310S, 19.00 percent, is 4.00 points above the nickel maximum of 309S, 15.00 percent. 310S also allows 1.50 percent silicon maximum against 0.75 percent in 309S. Carbon is the only composition difference between 310 and 310S.
Mechanical Properties of 309S, 310S and 310
309S, 310S and 310 have the same minimum mechanical values: 515 MPa tensile strength, 205 MPa yield strength, 40 percent elongation and 95 HRB hardness.
| Property | 309S | 310S | 310 |
|---|---|---|---|
| Tensile strength | 515 MPa min | 515 MPa min | 515 MPa min |
| Yield strength | 205 MPa min | 205 MPa min | 205 MPa min |
| Elongation | 40 % min | 40 % min | 40 % min |
| Hardness | 95 HRB max | 95 HRB max | 95 HRB max |
HRB is the Rockwell B hardness scale. The 309S and 310S values are for annealed material, which means softened by heat treatment. Strength does not separate the grades, so chemistry and temperature behaviour decide the choice.
Maximum Temperature of 309S and 310S
310S has a maximum service temperature in air of 1050 °C and resists scaling up to 1093 °C, while a producer gives 1000 °C as the maximum application temperature in air for 309S.
Scaling is the flaking oxide layer that forms on hot steel, and oxidation is the reaction with oxygen that forms it. The scaling figures are not service limits.
| Grade | Figure | What the figure measures |
|---|---|---|
| 309S | 1090 °C | Oxidation resistance up to this temperature; not a service limit |
| 309S | 1000 °C | Maximum application temperature in air, producer guidance |
| 310S | 1093 °C | Resists scaling up to this temperature; not a maximum temperature |
| 310S | 1050 °C | Maximum service temperature in air; suits intermittent heating |
A second producer states that 310S is best employed in high temperatures up to 1050 °C, with excellent oxidation resistance in mildly cyclic conditions. Cyclic means the part heats and cools repeatedly. A producer also states that 310S enhances oxidation and creep resistance beyond 309S.
The maximum depends on the atmosphere and the load. No scaling or service figure is printed for plain 310. Buyers can send the temperature, atmosphere and load to us before choosing a grade.
What Is the Difference Between 310 and 310S?
The difference between 310 and 310S is carbon: 310 allows 0.25 percent maximum and 310S allows 0.08 percent maximum.
Chromium and nickel ranges are the same in both grades, and so are the minimum mechanical values. The low carbon of 310S improves weldability. A producer lists ASTM A167 for 310 plate, sheet and strip.
The specification names the grade, and an enquiry should repeat it. 310S is the form whose carbon is limited for welded work.
Welding 309S and 310S
309S and 310S are the weldable low-carbon forms, because both limit carbon to 0.08 percent maximum.
ER310 is the filler named for welding 310S. No filler is named here for 309S or 310. The welding procedure and the producer data decide the wire.
Uses of 309S, 310S and 310
309S is used in furnace equipment and boiler parts, 310S in furnaces, kilns and radiant tubes, and 310 and 310S in heat-treatment equipment, burners and heat shields.
| Grade | Uses |
|---|---|
| 309S | furnace components, annealing boxes and bells, baffle plates, boiler baffles, thermowells, salt pots, salt bath treatment equipment, heat exchangers, refinery equipment exposed to thermal cycling |
| 310S | furnaces, kilns, radiant tubes, annealing covers; refractory supports, burner parts, conveyor belts, furnace linings, fans; heat-treatment baskets, heat exchangers, steam boilers; cement industry above 550 °C |
| 310 and 310S | furnace parts (linings, muffles, doors, baffles, radiant tubes); heat-treatment trays, baskets, fixtures and retorts; recuperators; burner parts and combustion chambers; kiln components, oven conveyors and liners; incinerators and waste-to-energy plants; heat shields in power generation; heater tube supports in petrochemical and refinery plants; high-temperature handling equipment in cement, steel and glass plants; exhaust and heat shield components in aerospace and automotive; cryogenic service where low-temperature toughness is needed |
Temperature limits depend on the atmosphere and the load, so every grade review starts with the duty.
How to Choose 309S, 310S or 310
Choose 310S for the higher chromium and nickel, intermittent high-temperature use and higher oxidation and creep resistance, and choose 309S for furnace equipment, annealing boxes and baffle plates.
| Duty | Grade to order |
|---|---|
| Furnaces, kilns, radiant tubes, burner parts | 310S |
| Intermittent high-temperature use | 310S |
| Oxidation and creep resistance beyond 309S | 310S |
| Furnace equipment, annealing boxes, baffle plates, thermowells | 309S |
| Welded fabrication | 309S or 310S |
| Specification names plain 310 | 310 |
| Temperature, atmosphere or load not known | Send the duty |
The higher nickel and chromium content of 310S adds to the cost of the material. Confirm temperature, atmosphere and load before moving from 310S to 309S.
A mill test certificate comes with every supply. The certificate reports the heat chemical analysis and the mechanical test results, so carbon, chromium and nickel can be compared with the table above. Quotations are made for a grade, size and quantity, and each grade has its own page: 309S stainless steel sheets and plates, 310S stainless steel sheets and plates and 310 stainless steel sheets and plates. Coil is on the 309S coils, 310S stainless steel coils and 310 coils pages.
The wider choice of heat-resisting grades is set out in stainless steel grades for high temperature, and the stainless steel grade selector narrows it by service. 410S, a chromium-only grade, is compared with 410 and 420 in 410, 410S and 420 compared.
Frequently Asked Questions
What Is the Difference Between 309S and 310S?
310S holds more chromium and nickel: 24.00 to 26.00 percent chromium and 19.00 to 22.00 percent nickel, against 22.00 to 24.00 and 12.00 to 15.00 percent in 309S. Both limit carbon to 0.08 percent maximum, and both carry minimum tensile strength of 515 MPa. 310S has a stated maximum service temperature in air of 1050 °C, and a producer gives 1000 °C as the maximum application temperature in air for 309S.
Can 309S Replace 310S to Save Cost?
No, not without checking the duty first. 310S has higher chromium and nickel, and a producer states that it enhances oxidation and creep resistance beyond 309S. Confirm temperature, atmosphere and load before any change of grade.
Is 1093 °C the Maximum Temperature of 310S?
No, 1093 °C is the temperature up to which 310S resists scaling. The maximum service temperature in air is 1050 °C, and the grade suits intermittent heating.
Which Filler Welds 310S?
ER310 is the filler named for 310S. Both 309S and 310S limit carbon to 0.08 percent maximum, which improves weldability.
Which Standard Covers 309S, 310S and 310?
ASTM A240/A240M covers plate, sheet and strip of chromium and chromium-nickel stainless steels. A producer lists ASTM A167 for 309 and 310 plate, sheet and strip, and not for 309S or 310S. Name the standard on the enquiry.
What Does a Mill Test Certificate Show for 309S and 310S?
A mill test certificate reports the heat chemical analysis and the mechanical test results. The percentages of carbon, chromium and nickel can then be compared with the grade limits. A certificate comes with every supply.