Skip to content
Ostrava Metals

Heat-resistant grades

Best Stainless Grades for High-Temperature Service

High-temperature stainless steel grades serve above about 550 °C, and the grades compared here are the austenitic 304, 309S, 310S, 321 and 347, the ferritic 430, 439 and 441, and the martensitic 410. Austenitic grades hold nickel, ferritic grades hold almost none, and martensitic grades are hardenable by heat treatment. No single temperature suits every grade, because each published figure measures something different.

High-temperature figures at a glance

Temperature figures, °C, scale 0 to 1100 °C

410650 °C continuous
430740 °C continuous
304, 321, 347816 °C code ceiling
441980 °C cyclic
309S1000 °C application
310S1050 °C intermittent
309S, oxidation resistance up to
1090 °C, not a service limit
310S, scaling resistance up to
1093 °C, not a service limit

Ferritic beats austenitic

  • Sulphur-bearing hot gas
  • Thermal shock
  • Low thermal expansion

Austenitic beats ferritic

  • Carburising and nitriding gas
  • Higher creep strength
Each figure measures something different. Atmosphere and load set the real limit, so send the temperature, atmosphere and load.

Creep strength is usually the main design factor above 550 °C. Creep is the slow stretching of metal under load at high temperature. Limits depend on the atmosphere, the load and the grade.

Which Temperature Figures Does Each Grade Have?

The published figures differ in meaning: some are service limits, some are scaling or oxidation limits, and one is a design-code ceiling.

Scaling is the flaking oxide layer that forms on hot steel, and oxidation is the reaction with oxygen that forms it. The table lists the figures printed here, with what each measures.

GradeFigureWhat the figure measures
304, 321, 347816 °C (1500 °F)ASME allowable stresses are given to this temperature; a code ceiling, not an oxidation limit
309S1000 °CMaximum application temperature in air, a producer states
309S1090 °COxidation resistance up to this temperature, Jindal states; not a service limit
310S1050 °CMaximum service temperature in air, intermittent
310S1093 °CScaling resistance up to this temperature, Jindal states; not a service limit
310S950 °CLimit when sulphur in the gas is above 2 g/m3
410650 °CSafe limit for continuous service, Jindal states; scaling is seen above it
430740 °CGood oxidation resistance, continuous service, Jindal states
430875 °CGood oxidation resistance, intermittent service, Jindal states
439850 to 950 °CRecommended service temperature, Jindal states
441980 °CUse up to this temperature, in particular for cyclic oxidation, Jindal states

For 304, 321 and 347 we found no official oxidation limit in air, so the code ceiling is the only figure printed.

Why Are 309S and 310S Chosen for Heat?

309S and 310S are austenitic grades whose high chromium and nickel give oxidation resistance.

310S has better oxidation and creep resistance than 309S, and the 309S and 310S compared guide gives their composition and both temperature figures. Sigma phase is a brittle phase that can form in austenitic steels after long exposure. A producer notes slight susceptibility to embrittlement for 310S in continuous operation at about 600 to 900 °C. The grade pages are 310S stainless steel sheets and plates and 309S stainless steel sheets and plates.

Why Are 321 and 347 Used at Heat?

321 and 347 are stabilised grades, which means titanium (321) or niobium (347) is added to tie up carbon, and they are used when parts spend time in the sensitising range, about 450 to 850 °C, during service or welding.

Jindal describes 321 as titanium-stabilised, for intergranular corrosion resistance in high-temperature use, and 347 is niobium-stabilised. Sensitisation is the formation of chromium carbides at the grain boundaries, which can happen during welding. The filler for 321 is ER347 and never ER321, as set out in the welding filler for stainless steel guide. The grade pages are 321 stainless steel sheets and plates and 347 stainless steel sheets and plates.

When Do Ferritic Grades Beat Austenitic Grades?

Ferritic grades beat austenitic grades in sulphur-bearing hot gases, in thermal shock and where thermal expansion must be low.

A producer states that ferritic stainless steels resist sulphur-containing hot gases and expand less. Ferritic steels are more resistant to thermal shock than high-temperature austenitic steels. Under reducing sulphur conditions a protective oxide needs chromium above 25 percent. Below that, low-melting nickel sulphides form, so a ferritic grade is chosen.

The ferritic grades with a published figure are 430 stainless steel sheets and plates, 439 stainless steel sheets and plates and 441 stainless steel sheets and plates. 410 stainless steel sheets and plates is martensitic and has the lowest figure in the table.

When Do Austenitic Grades Beat Ferritic Grades?

Austenitic grades beat ferritic grades in carburising and nitriding gases, and they have higher creep strength.

Carburising is the pick-up of carbon from the gas, and nitriding is the pick-up of nitrogen. Austenitic grades, with more nickel, are favoured over ferritic grades for carburising resistance.

How to Choose a High-Temperature Grade

The grade follows the atmosphere and the load first, and the temperature second.

DutyFamily to review
Sulphur-bearing hot gasFerritic
Carburising or nitriding gasAustenitic
High creep loadAustenitic
Repeated heating and coolingFerritic for thermal shock; 441 has a figure for cyclic oxidation
Parts welded in the 450 to 850 °C rangeStabilised: 321, 347
Temperature, atmosphere or load not knownSend the duty

The stainless steel grade selector narrows the choice by service. We send a mill test certificate with every supply, and buyers can send the temperature, atmosphere and load before a grade is chosen.

Frequently Asked Questions

What Counts as High-Temperature Service for Stainless Steel?

High-temperature service means above about 550 °C, where creep strength is usually the main design factor.

What Is the Temperature Limit of 321 and 347?

We found no official oxidation limit in air for 321 or 347. The only figure printed is the ASME code ceiling: allowable stresses are given to 1500 °F (816 °C), and that is a code ceiling, not an oxidation limit.

Does 430 Suit Continuous Service at 800 °C?

No, Jindal states good oxidation resistance for 430 up to 740 °C for continuous service and up to 875 °C for intermittent service. A continuous duty at 800 °C is above the continuous figure.

Which Stainless Grade Resists Sulphur in Hot Gas?

Ferritic grades resist sulphur-bearing hot gases. For 310S the limit falls to 950 °C when sulphur in the gas is above 2 g/m3. Under reducing sulphur conditions, chromium above 25 percent is needed for a protective oxide.

Does 441 Suit Cyclic Heating Up to 800 °C?

Yes, Jindal states 441 has good oxidation resistance, in particular cyclic oxidation, enabling use up to 980 °C. Cyclic means the part heats and cools repeatedly.

How Hot Can 410 Run in Service?

Jindal gives 650 °C as the safe limit for continuous service of 410, above which scaling is seen. We found no figure for 410S or 420 from any official source.

Is 310S Better Than 309S at High Temperature?

Yes, 310S has better oxidation and creep resistance than 309S. The 310S maximum service temperature in air is 1050 °C, intermittent, and a producer gives 1000 °C as the maximum application temperature in air for 309S.

Is Sigma Phase a Risk for 310S?

Yes, a producer notes slight susceptibility to embrittlement in continuous operation at about 600 to 900 °C.

Contact Ostrava Metals