Stainless steel welding filler is chosen from the base grade: 308L wire for 304L, 316L wire for 316L, 347 wire for 321 and 347, and 2209 wire for duplex 2205. Filler metal is the metal added to the joint, either as bare filler wire or rod, or as a coated electrode.
Welding filler by base grade
Base grade and wire class, AWS A5.9
- 304L: ER308L
- 316L: ER316L
- 321 and 347: ER347
- 309S: ER309Si
- 310S: ER310
- 2205: ER2209
Carbon steel to stainless
- To 304 or 304L, filler 309L
- To 316 or 316L, filler 309LMo
Rules to keep
- Carbon steel is never welded directly to austenitic
- The filler for 321 is ER347, never ER321
Most austenitic fillers are over-alloyed: they carry more chromium, nickel and molybdenum than the plate they join. Over-alloyed means carrying more alloy than the base metal. Duplex fillers carry about 2 to 4 percent more nickel. Carbon steel must never be welded directly to austenitic stainless steel.
What Do the Filler Codes Mean?
Two AWS (American Welding Society) standards classify most stainless steel filler: AWS A5.9 for bare wire and rod, and AWS A5.4 for covered electrodes.
AWS A5.9 covers bare stainless steel electrodes (wire and strip) for gas metal arc, submerged arc and other fusion processes, and wire and rods for gas tungsten arc and plasma arc welding. Classification is by chemical composition.
AWS A5.4 is the specification for stainless steel covered electrodes for shielded metal arc welding.
Gas tungsten arc welding is TIG, gas metal arc welding is MIG, and shielded metal arc welding is stick welding with a coated electrode.
ISO 14343 classifies wire and rod and ISO 3581 classifies covered electrodes. Producer datasheets print both codes beside each grade. In the tables the ER codes are AWS A5.9 wire and rod, and the E codes are AWS A5.4 electrodes.
Which Filler Suits Austenitic Grades?
Austenitic grades use a filler of matching type, with the L (low carbon) wire for the L grades.
Austenitic means the chromium-nickel family of stainless steel, such as 304L and 316L. The table lists the filler a producer's datasheet gives for each base grade.
| Base grade | Wire or rod (TIG, MIG) | Covered electrode |
|---|---|---|
| 304L | ISO 14343 S 19 9 L / AWS A5.9 ER308L | ISO 3581 E 19 9 L R / AWS A5.4 E308L-17 |
| 316L | ISO 14343 S 19 12 3 L / AWS A5.9 ER316L | ISO 3581 E 19 12 3 L R / AWS A5.4 E316L-17 |
| 317L | ISO 14343 S 19 13 4 L / AWS A5.9 ER317L | ISO 3581 E 19 13 4 L R / AWS A5.4 E317L-16 |
| 321 | ISO 14343 S 19 9 Nb / AWS A5.9 ER347 | ISO 3581 E 19 9 Nb R / AWS A5.4 E347-17 |
| 347 | ISO 14343 S 19 9 Nb / AWS A5.9 ER347; also S 19 9 Nb Si / ER347Si | ISO 3581 E 19 9 Nb R / AWS A5.4 E347-17 |
| 309S | ISO 14343 S 22 12 H / AWS A5.9 ER309Si | ISO 3581 E 22 12 R / AWS A5.4 E309-17 |
| 310S | ISO 14343 S 25 20 / AWS A5.9 ER310 | ISO 3581 E 25 20 B / AWS A5.4 E310-15 |
| 904L | ISO 14343 S 20 25 5 Cu L / AWS A5.9 ER385 | ISO 3581 E 20 25 5 Cu N L R / AWS A5.4 E385-16 |
The filler for 321 is ER347 and never ER321, because 321 and 347 are stabilised grades. Stabilised means titanium (321) or niobium (347) is added to tie up carbon. The low-carbon base metals are on the pages for 304L stainless steel sheets and plates and 316L stainless steel sheets and plates. The stabilised and heat-resistant base metals are on these pages:
What Filler Welds 304 and 316 That Are Not L Grades?
Plain 304 is welded with ER308/308L, ER308LSi or ER309 wire and E308/308L or E309 electrodes. Plain 316 takes G 19 12 3 L wire and E 19 12 2 electrodes in EN designations.
The EN designations for wire come from EN 12072 and for electrodes from EN 1600. We did not find an AWS code for non-L 316 in a read source, so none is printed. We found no verified filler for 201 or 202. The low-carbon grades are explained in low-carbon L grades.
Which Filler Welds Duplex and Super Duplex?
Duplex 2205 is welded with a 2209 filler, and S32750 super duplex with a 2594 filler.
| Base grade | Wire or rod (TIG, MIG) | Covered electrode |
|---|---|---|
| 2205 | ISO 14343 S 22 9 3 N L / AWS A5.9 ER2209 | ISO 3581 E 22 9 3 N L R / AWS A5.4 E2209-17; E 22 9 3 N L B / E2209-15 |
| S32750 | ISO 14343 S 25 9 4 N L / AWS A5.9 ER2594 | ISO 3581 E 25 9 4 N L R / AWS A5.4 E2594-16; E 25 9 4 N L B / E2594-15 |
Ferrite is one of the two phases in duplex steel, the other being austenite. Duplex fillers are over-alloyed in nickel, usually about 2 to 4 percent more than the wrought product. Welding duplex without filler is not recommended.
Modern duplex is balanced at 40 to 50 percent ferrite. The benefits need at least 25 to 30 percent ferrite. Preheating is not recommended for duplex as a general rule, and post-weld stress relief is not needed and may harm.
We found no verified filler for S32760, and it is not inferred from S32750. The base plate for the common duplex grade is on the duplex 2205 sheets and plates page.
What Filler Welds Ferritic and Martensitic Grades?
Ferritic and martensitic grades are listed in EN designations only: 430 takes G 17 or G 19 9 L wire, and 410 takes G 13 or G 19 9 L wire.
| Base grade | Wire (EN) | Electrode (EN) |
|---|---|---|
| 430 | G 17 or G 19 9 L | E 17 or E 19 9 L |
| 410 | G 13 or G 19 9 L | E 13 or E 19 9 L |
No AWS code for 410 or 430 was verified, so none is printed. 430 is ferritic, which means its structure is ferrite, and it needs controlled heat input to prevent grain growth. 410 is martensitic, which means its structure is martensite, a hard structure that forms on cooling. Martensitic grades are sensitive to cold cracking, which is cracking in the weld below about 400 °C. Preheat is heating the joint before welding. Preheat and post-weld heat treatment are normally required for martensitic grades. No temperature is printed here for 410.
Why Is Stainless Filler Over-Alloyed?
A sound austenitic weld normally holds a few percent of delta ferrite, which is a ferrite phase in the weld metal. Austenitic fillers are in most cases over-alloyed with chromium, nickel and molybdenum.
Sigma phase is a brittle phase that can form after long exposure between 550 and 900 °C in ferrite-bearing austenitic welds. Lower heat input is used on grades with about 25 percent chromium and 20 percent nickel, such as 310S, to limit that risk.
What Heat Input and Interpass Temperature Apply?
Heat input is set by the qualified welding procedure, and the producer figures here are the maximums stated on datasheets for each base grade.
Heat input is the energy put into the weld per millimetre of run, in kJ/mm. Interpass temperature is the metal temperature between two passes.
| Base grade | Heat input | Interpass | Preheat |
|---|---|---|---|
| 304L | under 2.0 kJ/mm | under 150 °C | none |
| 316L | under 2.0 kJ/mm | under 150 °C | none |
| 317L | under 1.5 kJ/mm | under 100 °C | none |
| 321 | under 1.5 kJ/mm | under 150 °C | none |
| 347 | under 1.5 kJ/mm | under 150 °C | none |
| 309S | under 2.0 kJ/mm | under 150 °C | none |
| 310S | under 1.0 kJ/mm | under 100 °C | not specified |
| 904L | under 1.0 kJ/mm | under 100 °C | none |
| 2205 | 0.5 to 2.5 kJ/mm | under 150 °C | none |
For 310S the datasheet adds that a string bead welding technique should be used. For super duplex, one producer states an interpass under 150 °C and another uses 100 °C, so the qualified welding procedure sets the limit.
Do 304 and 316 Need Preheating?
No, 304 and 316 are easy to weld and usually do not need preheating.
A producer datasheet states that no heat treatment is normally needed after welding 304L or 2205.
Can Carbon Steel Be Welded to Stainless Steel?
Yes, but only through an over-alloyed filler, because carbon steel must not be welded directly to austenitic stainless steel: the weld metal forms martensite.
The Australian welding standard AS/NZS 1554.6 gives 309L for carbon steel to 304 or 304L, and 309LMo for carbon steel to 316 or 316L. The shielding gas must not include the oxygen often used in carbon steel mixtures. Zinc must be removed from the heated zone of galvanised steel before welding.
The table lists the filler named for each dissimilar joint.
| Joint | Filler named |
|---|---|
| Carbon steel to 304 or 304L | 309L |
| Carbon steel to 316 or 316L | 309LMo |
| Duplex to austenitic stainless | AWS E309LMo or ER309LMo, frequently used |
| Duplex to carbon or low-alloy steel | AWS E309L or ER309L |
| 2205 to 304 or 316 | E2209, E309LMo |
Preheat of 150 °C applies to the carbon steel side only (over 0.2 percent carbon, or over 30 mm under high restraint), and never to the stainless side.
Which Shielding Gas Suits Stainless Steel?
Pure argon is the most common root gas (the gas on the back of the joint) for stainless steel, and hydrogen-containing mixtures must not be used for ferritic, martensitic or duplex grades.
The root gas may hold at most 20 ppm (parts per million) oxygen, and the argon purity should be at least 99.995 percent. For duplex TIG welding the gas is argon, argon with helium, or argon with 1 to 2 percent nitrogen.
How Is a Stainless Weld Cleaned?
A weld area must be clean, dry and free of carbon steel, zinc, paint, oil, grease and marking crayons before welding, and heat tint must be removed after it.
Weld tint marks the zones where the passive layer has been destroyed. Pickling removes high-temperature scale, and the part must be rinsed thoroughly. A non-stainless brush may leave iron particles that cause rust. The methods are in pickling and passivation after welding, and the corrosion types that follow poor cleaning are in types of stainless steel corrosion.
Send Us the Base Grade and Process
Buyers who name the base grade and the process can send the base grade and welding process to us. A mill test certificate comes with every supply.
Frequently Asked Questions
What Filler Welds 304L?
304L is welded with ER308L wire or E308L-17 electrodes. The ISO codes are S 19 9 L for wire and E 19 9 L R for electrodes. A producer datasheet gives under 2.0 kJ/mm and under 150 °C interpass.
What Filler Welds 316L?
316L is welded with ER316L wire or E316L-17 electrodes. The ISO codes are S 19 12 3 L and E 19 12 3 L R. The same datasheet gives under 2.0 kJ/mm and no preheat.
What Filler Welds 321?
321 is welded with ER347 wire or E347-17 electrodes, and never with ER321. The ISO codes are S 19 9 Nb and E 19 9 Nb R. Heat input is under 1.5 kJ/mm in the datasheet.
Can Carbon Steel Be Welded Directly to 304?
No, carbon steel must not be welded directly to austenitic stainless steel because the weld metal forms martensite. Use 309L filler for carbon steel to 304 or 304L, and 309LMo for carbon steel to 316 or 316L. Keep oxygen out of the shielding gas.
Does Duplex 2205 Need Preheating?
No, preheating is not recommended for duplex as a general rule. Interpass stays under 150 °C for standard and lean duplex. For super duplex the procedure sets it, 150 or 100 °C by producer. The qualified welding procedure sets the limit.
Do Hydrogen Gas Mixtures Suit Duplex?
No, hydrogen-containing mixtures must not be used for ferritic, martensitic or duplex stainless steel. Duplex TIG welds use argon, argon with helium, or argon with 1 to 2 percent nitrogen.
What Filler Joins Duplex 2205 to 304 or 316?
E2209 or E309LMo joins duplex 2205 to 304 or 316. AWS E309LMo or ER309LMo is frequently used to join duplex to austenitic grades. Check the choice against the qualified welding procedure.