The types of stainless steel corrosion are six: general, pitting, crevice, galvanic, intergranular and chloride stress corrosion cracking. Each has a different cause, and each has a grade or a practice that avoids it.
Six types of stainless steel corrosion
Where each type starts
General
- Uniform loss over the whole surface
Pitting
- Chlorides
Crevice
- Confined spaces
Galvanic
- Wet joint, two metals
Intergranular
- 450 to 850 °C, often from welding
Chloride SCC
- Above about 50 °C with tensile stress
Stainless steel resists corrosion through a thin chromium-rich passive layer. When the layer is damaged, one of the six types can start.
| Type | Where it attacks | Main cause |
|---|---|---|
| General | the whole surface | a medium that attacks the metal |
| Pitting | small spots on the surface | chlorides |
| Crevice | confined spaces | a gap that holds liquid |
| Galvanic | the joint between two metals | a wet joint with a potential difference |
| Intergranular | grain boundaries | 450 to 850 °C, often from welding |
| Chloride SCC | cracks under stress | chlorides above about 50 °C with tensile stress |
Why Does Stainless Steel Resist Corrosion?
Stainless steel resists corrosion through a thin chromium-rich passive layer that forms by itself when chromium is about 10.5 percent or more.
A passive layer is a thin surface layer that blocks further attack. Weld tint marks a zone where the passive layer has been destroyed, and pickling and passivation removes it.
What Is General Corrosion?
General corrosion is an even loss of metal over the whole surface, and a grade is usually regarded as resistant when the rate does not exceed 0.1 mm per year.
The rate depends on the medium and the grade. No corrosion rate for 304 in a named acid is given here; check the producer's data for that acid and temperature. The stainless steel grade selector narrows the choice by service.
What Is Pitting Corrosion?
Pitting corrosion is highly localised attack that leaves discrete pits on the surface, and chlorides are the usual cause.
Chlorides are salts such as sodium chloride in seawater and in many process liquids. Molybdenum and nitrogen in the grade raise resistance to pitting. 316 stainless steel sheets and plates carry molybdenum for this reason, and 904L and duplex carry more still.
What Is PREN and Why Does It Rank Grades?
PREN, the pitting resistance equivalent number, is calculated as %Cr + 3.3 x %Mo + 16 x %N, and a higher number means more resistance to pitting.
PREN is a ranking aid. The number does not describe a real environment and is not a guarantee. Cr is chromium, Mo is molybdenum and N is nitrogen. The PREN calculator works the sum for any composition, and stainless steel for seawater and chloride service gives the calculated and producer values for each grade.
What Is Crevice Corrosion?
Crevice corrosion is attack inside a narrow gap that holds liquid.
A grade with a higher PREN resists it better. Duplex 2205 sheets and plates and 904L stainless steel sheets and plates sit higher on the PREN scale than 316.
What Is Chloride Stress Corrosion Cracking?
Chloride stress corrosion cracking, or SCC, is cracking of 304 and 316 in chlorides above about 50 °C under tensile stress.
Tensile stress is a pulling stress, from loading or from residual stress left by welding and forming. SCC can occur lower, about 30 °C, in indoor swimming-pool air. No stainless steel grade is totally immune to chloride SCC. For chlorides above about 50 °C, duplex such as 2205 or a super duplex grade is the step up.
What Is Intergranular Corrosion?
Intergranular corrosion is attack along the grain boundaries, caused when chromium carbides form there after time in roughly 450 to 850 °C.
A grain boundary is the line where two metal crystals meet. The condition is called sensitisation, and it can happen during welding. Four remedies limit it:
- Use a low-carbon L grade.
- Use a titanium-stabilised grade (321) or a niobium-stabilised grade (347).
- Limit the time spent in the range.
- Solution anneal, which means heating to about 1,000 to 1,200 °C so that the carbides dissolve, followed by rapid cooling.
321 stainless steel sheets and plates are the titanium-stabilised choice. The filler for a 321 joint is in the welding filler for stainless steel guide.
What Is Galvanic Corrosion?
Galvanic corrosion needs three conditions: a wet joint, metal-to-metal contact and a meaningful difference in potential.
Potential is the electrical voltage a metal shows in the wet joint. The noble metal is the one with the higher potential, and the other metal corrodes.
Remove one of the three conditions and the attack stops. Insulate with suitable plastic strips, washers or sleeves, because paint is not a reliable insulator. Painting the noble metal 30 to 50 mm beyond the join also works.
The potential difference between passive 304 and passive 316 is small, so galvanic attack on 304 is not expected. With galvanised steel the zinc corrodes first. Galvanic effects are not generally serious when the wetted area of the corroding metal is 10 times that of the noble metal.
Which Grade Resists Each Type?
Each type has its own step-up: molybdenum grades for pitting and crevice, duplex for chloride SCC, and L or stabilised grades for intergranular attack.
| Type | First grade to check | Step-up |
|---|---|---|
| Pitting | 316 | 904L, duplex 2205, super duplex |
| Crevice | 316 | 904L, duplex 2205, super duplex |
| Chloride SCC | 304 or 316 (cracks above about 50 °C) | Duplex 2205 or super duplex |
| Intergranular | 304L or 316L | 321 (titanium) or 347 (niobium) |
| Galvanic | none; joint design decides | 304 against 316 is not expected to attack |
Which Test Detects Each Type of Corrosion?
ASTM A262 tests for intergranular attack, and ASTM G48 tests for pitting and crevice corrosion.
ASTM A262 covers five practices for detecting susceptibility to intergranular attack in austenitic stainless steels:
- A: oxalic acid etch
- B: ferric sulphate-sulphuric acid
- C: nitric acid
- E: copper-copper sulphate-sulphuric acid
- F: for molybdenum-bearing grades
Its results do not predict general corrosion, pitting or stress corrosion cracking.
ASTM G48 covers ferric chloride tests for pitting and crevice corrosion in oxidising chloride environments, in six methods, A to F:
- A: pitting
- B: crevice
- C and D: critical pitting and crevice temperature for nickel-base and chromium-bearing alloys
- E and F: stainless steels
A buyer who needs a test states the practice or method in the order.
Which Grade Suits Which Atmosphere?
430 suits interiors, 304 and 304L suit interiors and light urban air, and 316 and 316L suit urban air including light marine.
The 200 series sits lower: 201 has corrosion resistance comparable to 301, and 202 is comparable to 304 in moderately corrosive media. In harsher conditions the 200 series is lower than 304. The grade pages are 201 stainless steel sheets and plates and 304 stainless steel sheets and plates.
Ask Us About Your Duty
A mill test certificate comes with every supply from us. Send the grade and service to ask for a quotation.
Frequently Asked Questions
What Are the Types of Stainless Steel Corrosion?
The types are general, pitting, crevice, galvanic, intergranular and chloride stress corrosion cracking. Pitting and crevice corrosion are localised attack, usually in chlorides. Intergranular corrosion follows time in roughly 450 to 850 °C.
Can Stainless Steel Corrode?
Yes, stainless steel corrodes when its passive layer is damaged, in the six types listed. Chromium of about 10.5 percent or more forms the layer. Weld tint is one place where the layer has been destroyed.
Does 316 Resist Pitting Better Than 304?
Yes, 316 has a PREN of 22.6 against 17.5 for 304, calculated from minimum composition. Molybdenum is the difference. PREN ranks grades and does not guarantee behaviour in a real environment.
Can 304 and 316 Crack in Chlorides?
Yes, 304 and 316 can crack in chlorides above about 50 °C under tensile stress. Cracking can occur lower, about 30 °C, in indoor swimming-pool air. Duplex 2205 or a super duplex grade is the step up.
Is Any Stainless Steel Immune to Chloride SCC?
No, no stainless steel grade is totally immune to chloride SCC. Duplex and super duplex resist it better than 304 and 316. Super duplex should avoid prolonged exposure above 250 °C.
How Is Intergranular Corrosion Avoided After Welding?
Use a low-carbon L grade or a stabilised grade such as 321 or 347. Limit the time in the 450 to 850 °C range, or solution anneal at about 1,000 to 1,200 °C (heating so that the carbides dissolve) and cool rapidly.
Does Galvanic Corrosion Affect 304 Bolted to 316?
No, the potential difference between passive 304 and passive 316 is small, so galvanic attack on 304 is not expected. Galvanised steel is different: the zinc corrodes first. Insulate with plastic strips, washers or sleeves.
What Does ASTM A262 Test?
ASTM A262 tests for susceptibility to intergranular attack in austenitic stainless steels, through five practices A, B, C, E and F. The results do not predict general corrosion, pitting or stress corrosion cracking.