Pickling removes a thin layer of metal from the stainless steel surface with acid, and passivation helps form the protective passive layer on a clean surface. After welding, pickling removes the heat tint, and passivation is optional after a proper pickle.
Pickling and passivation after welding
Order of work on a welded part
- Degrease the weld area
- Pickle to remove the heat tint
- Rinse with de-ionised water
- Passivate where the specification asks
- Test for free iron
Pickling
- Removes a thin layer of metal and weld heat tint
- Nitric and hydrofluoric mixtures usually
- First on a welded part
Passivation
- Removes free iron and forms the passive layer
- Nitric acid widely, citric acid can also help
- Optional after a proper pickle
Steel from mills and reputable stockholders is already fully passive. Acid passivation is the exception, not the rule. A welded or fabricated part is different, because heat from the weld and contact with workshop tools change the surface.
Stainless steel pickling and passivation have no single acid strength, bath temperature or time that fits every job. The work follows ASTM A380/A380M (cleaning, descaling and passivation practice), ASTM A967/A967M (chemical passivation treatments) and the supplier's data sheet. Sources quote different strengths, so none is printed.
What Are Descaling, Pickling and Passivation?
Descaling removes scale, the oxide layer formed by heat. Pickling removes a thin layer of metal, and passivation helps form the passive layer on a clean surface.
The passive layer is a thin film that protects stainless steel from corrosion. Chromium in the steel forms it.
What Is Pickling of Stainless Steel?
Pickling is the removal of a thin layer of metal from the surface with acid. Mixtures of nitric and hydrofluoric acids are usually used.
Pickling removes weld heat tint, where the surface chromium is reduced. Heat tint is the colour left by welding, and the colours range from pale straw to dark blue. Removing the affected layer of metal exposes steel that has its full chromium content again.
What Is Passivation of Stainless Steel?
Passivation removes free iron from the surface and helps form the passive layer. Nitric acid is widely used. Weaker oxidising acids such as citric acid can also help form the passive layer.
Before passivation the surface must be descaled, free of any chromium-depleted (low-chromium) layer removed by pickling, and clean of oil, grease and lubricants. Nitric acid alone cannot be relied on to remove heat tint.
What Is the Difference Between Pickling and Passivation?
Pickling removes a thin layer of metal, and passivation helps form the passive layer on the clean surface. Pickling comes first on a welded part, and passivation follows on the clean surface.
| Item | Pickling | Passivation |
|---|---|---|
| What it does | Removes a thin layer of metal and weld heat tint | Removes free iron and helps form the passive layer |
| Acid | Nitric and hydrofluoric mixtures usually | Nitric acid widely; citric acid can also help |
| Order on a weld | First | After a clean surface is reached |
| After a proper pickle | Done | Optional |
Do You Need Both After Welding?
No, good practice after welding is to remove all visible heat tint by pickling, and passivation is optional after a proper pickle. The heat tint ranges from pale straw to dark blue, and hidden weld faces need it removed too.
Degrease the area before removing heat tint. Where a drawing or customer specification calls for passivation, follow ASTM A967/A967M.
What Are the Methods of Pickling?
Four methods are used:
- Tank immersion is done off site and is best on health and safety grounds.
- Spray pickling can be done on site, but only by specialists with safety and acid-disposal equipment.
- Circulation pickling is recommended for pipework carrying corrosive liquids.
- Brush-on pastes or gels and electrochemical cleaning suit welds and other small areas.
Contact times vary by grade, so follow the supplier's instructions. Excessive contact time can cause pitting. Pitting is small holes eaten into the surface. De-ionised water is normally used for the final rinse.
Who Should Do Pickling and Passivation?
Tank immersion, spray pickling and nitric passivation should go to competent fabricators or finishing specialists. Nitric and hydrofluoric products should be avoided where a surface only needs decontamination. Decontamination means cleaning off surface contamination without removing metal.
Why Does Iron Contamination Matter?
Carbon steel tooling and mixed-metal shops contaminate stainless steel with iron.
The ferroxyl test detects free iron or iron oxide. ASTM A380/A380M gives the procedure, using nitric acid, distilled water and potassium ferricyanide. No pass criteria are printed here, because the acceptance limit belongs to the order or the specification.
What About Electropolished Surfaces?
Electropolished surfaces are passive and corrosion-resistant. ASTM B912 and ISO 15730 cover electropolishing and passivation.
Electropolishing for food and pharma equipment is covered in stainless steel for food and pharma equipment.
Order of Work After Welding
The steps run in a fixed order on a welded part:
- Degrease the weld area.
- Pickle to remove the heat tint, including on hidden weld faces.
- Rinse with de-ionised water.
- Passivate where the specification asks.
- Test for free iron with the ferroxyl test.
Welded work in 304 sheets and plates and 316L sheets and plates follows the same order. A mill test certificate comes with every supply.
Send the Drawing and Grade
Send the drawing and grade to us, and we reply with a quotation for the sheet or plate.
Frequently Asked Questions
Which Acids Are Used for Pickling and Passivation?
Pickling usually uses mixtures of nitric and hydrofluoric acids. Passivation uses nitric acid, and weaker oxidising acids such as citric acid can also help.
Do You Pickle Before Passivating?
Yes, pickle first where heat tint or scale is present. Passivation needs a descaled, clean surface, and chromium-depleted layers must be removed by pickling before it.
Why Remove Heat Tint After Welding?
Heat tint marks a surface where the chromium is reduced. Good practice is to remove all visible heat tint, from pale straw to dark blue, including on hidden weld faces.
Can Citric Acid Be Used for Passivation?
Yes, citric acid can help form the passive layer, as can other weaker oxidising acids, although nitric acid is widely used. Follow the specification and the supplier's instructions.
Which Water Is Used for the Final Rinse?
De-ionised water is normally used for the final rinse. Contact times vary by grade, so follow the supplier's instructions.
Is Passivation Always Needed?
No, acid passivation is the exception, not the rule. Steel from mills and reputable stockholders is fully passive, and passivation is optional after a proper pickle.
Which Standards Cover Pickling and Passivation?
ASTM A380/A380M covers cleaning, descaling and passivation practice, and ASTM A967/A967M covers chemical passivation treatments. Acid strength and time follow the supplier's data sheet.