Food grade stainless steel is a use description, not a grade, and 304 and 316L are two grades used for food and pharma equipment. There is no single official food grade list, and no US Food and Drug Administration (FDA) rule names a grade. The rules ask that food-contact surfaces are corrosion-resistant and non-toxic, with seams that do not collect food particles.
304 against 316L for food equipment
304
- Carbon 0.07 max
- No molybdenum requirement stated
- About 200 ppm chloride
316L
- Carbon 0.030 max
- Molybdenum 2.00 to 3.00
- 316 takes about 1,000 ppm chloride
- Large product contact areas
- 0.8 micrometre Ra or lower
- Cold-rolled up to 4 mm
- Usually needs no polishing
316L is used where chloride, sulphur dioxide or salty food contact is heavier, and for welded equipment. 304 is used extensively in food and beverage preparation because it remains inert in many food environments.
What Does Food Grade Stainless Steel Mean?
Food grade stainless steel means stainless steel used where it touches food, and no single official list defines which grades qualify.
The US federal rule for food plants, 21 CFR 117.40 (Title 21 of the Code of Federal Regulations), says food-contact surfaces must be corrosion-resistant when in contact with food. Surfaces must be made of non-toxic materials designed to withstand the environment of their intended use. Seams on food-contact surfaces must be smoothly bonded or maintained so as to minimise accumulation of food particles. The rule names no grade.
Regulation (EC) No 1935/2004 covers food contact materials. Under normal or foreseeable conditions of use, such materials must not transfer constituents to food in quantities that could endanger human health. Nor may they bring about an unacceptable change in the composition of the food or a deterioration in its organoleptic characteristics. Organoleptic means affecting taste, smell or appearance.
A Council of Europe guide on metals is not legally binding and serves as a reference for Article 3(1) of the regulation. The guide states that all stainless steel families can be used as food contact materials, and suggests labelling and cleaning instructions for acidic, alkaline or salty foods. France requires at least 13 percent chromium for food-contact stainless steel, and Italy keeps a positive list of approved grades.
Is 304 Stainless Steel FDA Approved?
No, no FDA text names 304 or any other grade as approved.
The FDA rule is functional: it describes what the surface must do, not which steel to use. A mill test certificate reports chemistry and mechanical test results, not an FDA status.
Which Is Better for Food Equipment, 304 or 316L?
304 is used extensively in food and beverage preparation, and 316L is used where chlorides, sulphur dioxide or heavy welding are involved.
| Grade | Carbon (%) | Molybdenum (%) | Food and pharma use |
|---|---|---|---|
| 304 | 0.07 max | none listed | Food and beverage preparation, brewing, dairy |
| 304L | 0.030 max | none listed | Tanks, pressure vessels, welded structures in food industries |
| 316L | 0.030 max | 2.00 to 3.00 | Extensive welding in food processing and pharmaceutical manufacturing |
316L holds 2.00 to 3.00 percent molybdenum, and it resists high chloride or sulphur dioxide, for example in white wine, salty foods and pectin. 430 is a ferritic grade, which means its structure is ferrite and it holds almost no nickel. 430 has acceptable corrosion resistance, but it is less easily formed or welded than austenitic grades such as 304 and 316L. Where welding ferritic grades is unavoidable, use titanium or niobium stabilised grades such as 441.
Pages for 304 stainless steel sheets and plates and 316L stainless steel sheets and plates carry the full composition and strength.
Why Do Welded Food Plants Use L Grades?
Welded food plants use L grades because low carbon limits chromium carbide formation in the weld zone.
L means low carbon, 0.030 percent maximum in 304L and 316L. Chromium carbides form at grain boundaries in about 450 to 850 °C and reduce corrosion resistance. Heating 304, up to 0.07 percent carbon, to about 980 to 1,180 °C after welding and cooling rapidly redissolves the carbides. Low-carbon 304L and 316L have much improved weld corrosion resistance. 316L allows welding without post-weld heat treatment. Compare the two L grades in low-carbon 304L and 316L compared.
Which Stainless Steel Grade Suits Pharma Equipment?
No document we found names a single grade for pharma. 316L is used for extensive welding in pharmaceutical manufacturing and food processing, and ASME BPE covers bioprocessing equipment.
What Surface Roughness Do Hygienic Surfaces Need?
A hygienic design guideline recommends that large product contact areas have 0.8 micrometre Ra or lower, where Ra is the average roughness of a surface in micrometres.
Cold-rolled stainless steel up to 4 mm thick usually needs no polishing, but thicker sheet may need polishing. The roughness of each mill finish is in stainless steel surface finishes.
EN 1672-2 sets hygiene and cleanability requirements for food processing machinery and its components, and it names no grade. ASME BPE covers the materials, design, fabrication, inspection, testing and certification of bioprocessing equipment. No roughness figure from either document is printed here.
What Is Electropolishing and Why Is It Used?
Electropolishing is an electrochemical process in which the workpiece is the anode and metal is removed ion by ion, and it gives a smooth, passive surface.
The process can reduce Ra by about half, and about 5 to 10 micrometres of metal is removed. The surface carries no foreign material from polishing. Standards for it include ISO 15730 and ASTM B912. The table gives a typical bath.
| Parameter | Typical value |
|---|---|
| Solution | equal volumes of 96 percent sulphuric acid and 85 percent orthophosphoric acid |
| Current density | 5 to 25 A/dm2 |
| Temperature | 40 to 75 °C |
| Time | 2 to 20 min |
When Is Passivation Needed After Pickling?
Passivation is needed when the specification calls for it, and it is optional after a proper pickle.
Passivation removes free iron. Pickling is an acid treatment that removes weld scale and heat tint. Follow ASTM A380/A380M, which covers recommendations and precautions for cleaning, descaling and passivating stainless steel parts, and ASTM A967/A967M, which covers several chemical passivation treatments, with the supplier's data sheet. Pickling and passivation of stainless steel sets out when each is needed after welding.
How Much Chloride Can 304 and 316 Take?
304 takes about 200 ppm (parts per million) chloride and 316 about 1,000 ppm, for continuous exposure at neutral pH and ambient temperature, as the Australian stainless industry body gives them.
Free chlorine limits are about 2 ppm for 304 and about 5 ppm for 316 at about 20 °C and neutral pH. The figures depend on the grade, the duty and the procedure, and they are not standard values. Chlorine attack can occur with bleach-laden washdown water if pools form in drains that are usually empty.
Stress corrosion cracking of 304 and 316 in chloride needs tensile stress and a temperature above about 50 °C. Pitting and crevice attack are explained in types of stainless steel corrosion. Utensil grades and the Indian utensil standards are covered in stainless steel for kitchenware and utensils.
What Does a Supply for Food Equipment Include?
A mill test certificate comes with every supply, and it reports the chemical analysis of the heat and the mechanical test results.
We supply 304 and 316L sheets and plates from Mumbai. We can quote against your drawing if you send the product, cleaning agent and finish.
Frequently Asked Questions
What Is Food Grade Stainless Steel?
Food grade stainless steel is stainless steel used where it touches food. No official list of food grades exists. The FDA rule and Regulation (EC) No 1935/2004 describe what the surface must do, and name no grade.
Which Rules Apply in the EU?
Regulation (EC) No 1935/2004 requires that food contact materials do not transfer constituents to food in quantities that could endanger health. A Council of Europe guide states all stainless families can be used, and it is not legally binding.
Do National Rules Set Limits on Stainless Steel?
Yes, in some countries. France requires at least 13 percent chromium for food-contact stainless steel, and Italy keeps a positive list of approved grades.
Can Bleach Damage Stainless Steel Equipment?
Yes, chlorine attack can occur with bleach-laden washdown water if pools form in drains that are usually empty. About 2 ppm free chlorine is the figure given for 304 and about 5 ppm for 316 at 20 °C and neutral pH.
What Is ASME BPE?
ASME BPE covers the materials, design, fabrication, inspection, testing and certification of bioprocessing equipment. Read the current edition for the requirements of the project.
Does Electropolishing Reduce Surface Roughness?
Yes, electropolishing can reduce Ra by about half, and the surface carries no foreign material from polishing. The process removes about 5 to 10 micrometres of metal.
Which ASTM Standards Cover Passivation?
ASTM A380/A380M covers cleaning, descaling and passivating practice, and ASTM A967/A967M covers chemical passivation treatments. ASTM B912 covers passivation of stainless steels using electropolishing.