Stainless steel for kitchenware uses 304, 202, 201 and 430. 304 holds 8.0 to 10.5 percent nickel, 430 is magnetic and is used as the base layer of induction cookware, and 202 and 201 hold less nickel and cost less. The common labels 18/8 and 18/10 both point to the 304 family, and 18/0 points to 430. The grade, not the label, sets the nickel content, magnetism and corrosion behaviour.
Kitchen grades by nickel
Nickel, % by weight, scale 0 to 12 %
- 18/8 and 18/10
- Both point to the 304 family
- 18/0
- Points to 430, which is magnetic
In India, utensil sheet is covered by the BIS standards IS 5522 and IS 15997. As of 1 November 2026, enforcement of the Quality Control Order (QCO) for them is not operative up to 31 March 2027, and BIS and IS 6911 compliance gives the dates.
What Do 18/8, 18/10 and 18/0 Mean?
18/8 means 18 percent chromium and 8 percent nickel, and it is the 304 grade.
Austenitic and ferritic are the two crystal structures that matter here. Austenitic grades such as 304 hold nickel. Ferritic grades such as 430 hold almost none.
The British stainless industry body explains the labels as follows. 18/8 is austenitic, so a magnet does not attract it, or attracts it only very weakly. 18/10 is essentially 304 as well: the 10 does not show a higher nickel content and is a marketing label. 18/0 is the 430 grade. The chromium in 18/0 is said to be 18 percent but is nearer 17 percent, and it is ferritic, so a magnet attracts it.
Which Grades Are Used for Kitchen Utensils?
304, 202, 201 and 430 are four grades used for kitchen utensils, and they differ mainly in nickel.
| Grade | Chromium (%) | Nickel (%) | Typical kitchen use |
|---|---|---|---|
| 304 | 17.5 to 19.5 | 8.0 to 10.5 | Utensils, cookware, sinks, appliances, food-handling equipment |
| 202 (Jindal J202) | 17.00 to 19.00 | 4.0 to 6.0 | Cookware, sinks |
| 201 | 16.0 to 18.0 | 3.50 to 5.50 | Cooking utensils, catering equipment, small appliances |
| 430 | 16.00 to 18.00 | 0.75 max | Kitchen equipment, appliances, decorative trims, dishwashers, stove trims, sinks |
The values for 202 are Jindal limits for its J202 grade. The 201 limits are for 201 in general. Our pages cover 304 stainless steel sheets and plates, 202 stainless steel sheets and plates, 201 stainless steel sheets and plates and 430 stainless steel sheets and plates.
How Do 202, 201 and 430 Compare with 304 for Corrosion?
304 resists corrosion better than 202 and 201, and the gap shows in harsher conditions; 430 is adequate for everyday kitchen use, but not recommended for direct cooking contact.
Low-nickel 200-series grades have less corrosion resistance than grade 304. Jindal states that 202 is comparable to 304 in moderately corrosive media, and 202 has lower corrosion resistance than 304 in harsher conditions. Jindal states that 201 offers corrosion resistance comparable to 301-grade stainless steel, which is not the same as 304.
430 has moderate corrosion resistance and good oxidation resistance, and it is adequate for everyday kitchen use, but not recommended for direct cooking contact.
Does Induction Cooking Need Magnetic Steel?
Yes, induction cooking needs magnetic material, and 430 is commonly used as the exterior base layer of induction-compatible cookware.
Induction cooking only works with ferromagnetic material, meaning material a magnet attracts. Annealed 304 is austenitic and shows no magnet pull. Jindal states the 430 use as a base layer and does not recommend 430 for direct cooking contact.
Can a Magnet Identify the Grade?
No, a magnet alone does not identify the grade.
Annealed 304 shows no pull, but welded 304 often attracts a magnet lightly even though the base is non-magnetic. 430 is magnetic. A magnet result for 201 or 202 is not given.
Some austenitic grades may become mildly magnetic after cold working, depending on composition.
How Does Jindal J4 Draw Compared with 304?
Jindal J4, a low-nickel Jindal 200-series grade, has a limiting drawing ratio of 1.7 against 2.1 for 304, and an Erichsen cupping depth of 11.5 mm against 13.1 mm.
Drawing is the process of forming a flat blank into a cup or pot. The limiting drawing ratio is the largest ratio of blank diameter to cup diameter that forms without tearing. A higher limiting drawing ratio allows a deeper draw in one step. Erichsen cupping depth is a test that measures how far a sheet stretches before it cracks, and for IS 5522 it is by agreement between purchaser and manufacturer. The figures in the table are from Jindal's 200-series brochure.
| Property | 304 | Jindal J4 |
|---|---|---|
| Limiting drawing ratio | 2.1 | 1.7 |
| Erichsen cupping | 13.1 mm | 11.5 mm |
Which Indian Standards Cover Utensil Sheet?
IS 5522 covers stainless steel sheets and strips for utensils, and IS 15997 covers low-nickel austenitic stainless steel sheet and strip for utensils and kitchen appliances.
The BIS manual for IS 5522 groups the grades: Group 1 is austenitic 304 and 302, and Group 2 is ferritic 430. Three other standards cover finished utensils and composite material: IS 14756 for finished stainless steel utensils, IS 15960 for composite bottom cooking utensils and IS 18755 for tri-ply stainless steel and aluminium material.
Suspension of the QCO is not repeal, and a buyer may still ask for BIS-marked utensil sheet. Orders change, so confirm the current status at steel.gov.in and bis.gov.in.
Does Stainless Steel Release Metals Into Food?
Yes, in trace amounts: Jindal states that chromium, iron and nickel may migrate into food, generally well below established safety limits.
People with diagnosed nickel sensitivity may prefer nickel-free cookware. Food-contact rules, cleaning and finish for equipment are covered in stainless steel for food and pharma equipment.
How Does Cost Compare Between Kitchen Grades?
430 costs less than 304 because it lacks nickel, and 202 is more affordable than 304 because of its reduced nickel.
Nickel is 0.75 percent maximum in 430, 4.0 to 6.0 percent in 202 and 8.0 to 10.5 percent in 304. The factors behind price are in stainless steel price factors. For current rates see the 430 sheet price list and the Jindal sheet price list.
We supply 304, 202, 201 and 430 sheets and plates from Mumbai, and a mill test certificate comes with every supply. We can quote once you send the utensil, thickness and quantity.
Frequently Asked Questions
Which Stainless Steel Grade Is Used for Utensils?
304 is used for food-contact utensils, 430 for magnetic and non-contact parts, and 202 and 201 where cost matters. The Indian standard for utensil sheet, IS 5522, groups 304 and 302 in Group 1 and 430 in Group 2.
Is 18/10 Better Than 18/8?
No, 18/10 is essentially 304, the same grade as 18/8. The 10 is a marketing label and does not show a higher nickel content. Grade 304 carries 8.0 to 10.5 percent nickel.
What Is the Difference Between 304 and 202?
304 has 8.0 to 10.5 percent nickel and 202 (Jindal J202) has 4.0 to 6.0 percent. Lower nickel makes 202 more affordable, and 202 has lower corrosion resistance than 304 in harsher conditions.
Does 18/0 Stainless Steel Work on Induction Hobs?
Yes, as a magnetic base layer. 18/0 is the 430 grade, which is ferritic and attracted by a magnet. Jindal does not recommend 430 for direct cooking contact.
How Well Does 430 Form for Deep Drawing?
430 has good cold formability but is less formable than austenitic grades. No drawing ratio for 430 is published here, so ask us with the part drawing.
Which Standard Covers Finished Utensils?
IS 14756 covers finished stainless steel utensils. IS 15960 covers composite bottom cooking utensils, and IS 18755 covers tri-ply stainless steel and aluminium material.
Is a Magnet Test Reliable for Stainless Steel?
No, a magnet alone does not identify the grade. Annealed 304 shows no pull, welded 304 often attracts a magnet lightly, and 430 is magnetic.