Duplex steel for oil and gas is chosen for its strength and chloride resistance, with duplex 2205 for general offshore duty and super duplex S32750 and S32760 where pressures and chloride loads are higher. Duplex stainless steel has a mixed structure of ferrite (a structure that holds almost no nickel) and austenite (a structure that holds nickel), about 40 to 50 percent ferrite in modern grades. The standards, temperature limits and welding rules decide whether a grade can be used.
Duplex temperature ranges
Temperature range, °C, scale 0 to 1000 °C
- Duplex 2205 service
- -40 to 300 °C
- Super duplex S32750 and S32760
- Avoid prolonged exposure above 250 °C
Duplex 2205 has a minimum yield strength of 450 MPa, about twice the yield strength of 304 and 316.
Where Is Duplex Used in Oil and Gas?
Duplex and super duplex are used for firewater and process piping, heat exchangers, pumps, pipework and blast walls on offshore installations.
| Grade | Uses |
|---|---|
| Duplex 2205 | Oil and gas, petrochemical, heat exchangers, desalination |
| Super duplex S32750 | Offshore platforms (heat exchangers, process and service water, firefighting, injection and ballast water), oil and gas, petrochemical pumps and pipework, desalination |
| Super duplex S32760 | Seawater and offshore systems, oil and gas, desalination |
Super duplex has been used in fire-suppression and process water piping on offshore oil production rigs. A producer states that super duplex 2507 (S32750) suits high pressures and is specified for deep and ultra-deep umbilicals, and that duplex has been used for blast walls.
| Grade and form | Maximum hardness |
|---|---|
| Super duplex S32750 plate | 32 HRC (Rockwell C scale) |
The grades are duplex 2205 sheets and plates, super duplex S32750 sheets and plates and super duplex S32760 plates, and duplex and super duplex compared sets the families side by side.
What Does NORSOK M-001 Cover?
NORSOK M-001, Materials selection, concerns hydrocarbon production and processing facilities and supporting systems for fixed offshore installations, including subsea production systems.
NORSOK is the Norwegian petroleum standards family. M-001 also applies to onshore terminals, except structural and civil works. The basis of M-001 is a minimum 20 years design life. The duplex rules inside M-001 are not printed here; read the current edition for the duty.
What Is NORSOK M-650?
NORSOK M-650 sets qualification requirements for manufacturers of special materials, and it applies to duplex stainless steel of all grades, product forms and dimensions. M-650 also applies to high-alloy austenitic stainless steel and to nickel-base alloy and titanium castings. M-650 qualifies the manufacturer, not the heat, so ask for the mill's status in the enquiry.
What Does Sour Service Mean for Duplex?
Sour service is service in oil and gas that contains hydrogen sulphide (H2S), which can crack susceptible metals.
Duplex grades are less sensitive than austenitic grades to sulphide stress cracking, which is cracking caused by hydrogen sulphide, and to hydrogen embrittlement. A producer lists duplex 2205 and super duplex 2507 among grades included in ISO 15156-3, the part of the sour service standard ISO 15156 that covers corrosion-resistant alloys. The permitted conditions are in the current edition of ISO 15156, and no limit is printed here. Check the edition against the project before ordering.
What Is the Upper Temperature for Duplex Steel?
Duplex 2205 is used from -40 °C to 300 °C, and super duplex S32750 and S32760 should avoid prolonged exposure above 250 °C.
Prolonged exposure above 250 °C changes the microstructure of super duplex and lowers impact strength. The upper limit for duplex service is controlled by the formation of alpha prime, the brittle phase behind 475 °C embrittlement. Pressure vessel codes set their own limits by grade and code.
What Causes Embrittlement and Sigma Phase?
Embrittlement comes from brittle phases that form when duplex steel stays in certain temperature ranges.
| Phase or effect | Temperature range |
|---|---|
| 475 °C embrittlement | about 300 to 525 °C |
| Nitrides and carbides | about 450 to 800 °C |
| Sigma phase, duplex 2205 | about 700 to 950 °C |
| Sigma phase, super duplex 2507 | about 700 to 1000 °C |
475 °C embrittlement is the name of the effect, not a limit. Sigma phase is a brittle intermetallic phase. Sigma is most likely when cooling during manufacture or welding is too slow, and it causes loss of impact toughness and reduces corrosion resistance.
ASTM A923 has three test methods for detecting detrimental intermetallic phase in duplex steels: a sodium hydroxide etch, a Charpy impact test and a ferric chloride corrosion test. ASTM A923 gives about 320 to 955 °C as the range in which intermetallic compounds can form on exposure.
How Is Duplex Steel Welded for Offshore Work?
Duplex steel is welded with controlled heat input, low interpass temperature and matched filler, and the qualified welding procedure sets the limits.
Heat input for duplex 2205 is about 0.5 to 2.5 kJ/mm, and the interpass temperature is under 150 °C. The filler table, the shielding gas and the dissimilar joints are in welding filler for stainless steel.
Duplex can tolerate relatively high heat input. Too little gives excess ferrite and loses toughness and corrosion resistance. Too much risks intermetallic phases. Interpass temperature is the temperature of the weld between passes.
Preheating is not recommended for duplex as a general rule. Post-weld stress relief is not needed and may harm. Heat treatment above 315 °C risks detrimental phases. Where heat treatment is needed, use full solution annealing (heating so that unwanted phases dissolve) and a water quench.
Modern duplex is balanced to 40 to 50 percent ferrite. The benefits are reached at 25 to 30 percent ferrite or more. That figure is for parent metal, not a weld acceptance limit.
How Is Duplex Cleaned After Fabrication?
ASTM A380/A380M covers cleaning, descaling and passivating of stainless steel parts, and ASTM A967/A967M covers chemical passivation treatments. Pickling paste makes a hazardous solution when rinsed. Pickling removes scale and passivation removes free iron; both are explained in pickling and passivation of stainless steel.
Which Documents Come with Duplex Plate?
A mill test certificate comes with every supply, reporting the chemical analysis of the heat and the mechanical test results.
We supply duplex 2205 and super duplex S32750 and S32760 plate from Mumbai. We can take the project specification and quote against it.
Frequently Asked Questions
Is Duplex Steel Listed for Sour Service?
Yes, in listed conditions. A producer lists duplex 2205 and super duplex 2507 among the grades included in ISO 15156-3. The permitted conditions are in the current edition, so check them against the duty.
What Is the Maximum Temperature for Duplex 2205?
Duplex 2205 is used from -40 °C to 300 °C. The upper limit is controlled by alpha prime formation, and pressure vessel codes set their own limits by grade and code.
Does Super Duplex Need Preheating Before Welding?
No, preheating is not recommended for duplex as a general rule. Heat input and interpass temperature are controlled instead, and the qualified welding procedure sets the limits.
What Is 475 °C Embrittlement?
475 °C embrittlement is a loss of toughness that can occur in duplex steel in about 300 to 525 °C. The number names the effect and is not a service limit.
What Is NORSOK M-650?
NORSOK M-650 sets qualification requirements for manufacturers of special materials, including duplex stainless steel of all grades. The qualification covers the manufacturer, not the heat.
Does Duplex Replace 316L Offshore?
Yes, in some systems. A producer states that duplex 2304, a duplex grade used for firewalls, gives weight and cost reduction against 316L for firewalls. The system, pressure and chloride load decide the grade.
Can Duplex Steel Be Stress Relieved After Welding?
No, post-weld stress relief is not needed and may harm. Heat treatment above 315 °C risks detrimental phases. Where treatment is needed, use full solution annealing and a water quench.